Selection parameters

Validation
hybrid filler design

01Validation route

Confirm the matrix, target properties and process window, then select surface treatment, run a dosage gradient and retest performance. Published data does not replace customer-specific validation.

APPLICATION EVIDENCE

Application test data

These records relate to this application. Formulations, loadings and conditions differ; review the complete comparisons.

3 data tablesPA6: whisker, glass-fibre and wollastonite comparisons

The 15% glass-fibre + 15% whisker group has higher strength but lower elongation and unnotched impact than the 30% glass-fibre group. Three source tables are kept separate.

These three comparisons use different formulations and units and must not be ranked across tables. The first says nylon without a PA grade; the second specifies unactivated whiskers; the third compares equal loadings of whiskers and wollastonite.

Swipe to compare all columns ↔

Nylon: unfilled versus 30% whisker
PropertyStandard / conditionUnitBlank30%
Tensile strengthD638kg/cm²635835
Tensile modulusD638kg/cm²2.33×10⁴4.53×10⁴
Flexural strengthD790kg/cm²8791208
Flexural modulusD790kg/cm²2.13×10⁴4.03×10⁴
Notched impact strengthD256kgf·cm/cm4.723.4
Heat deflection temperatureD648°C6590.5

Swipe to compare all columns ↔

PA6: 15% glass fibre + 15% unactivated whisker versus 30% glass fibre
PropertyUnit100% PA6PA6 + 15% GF + 15% CSWPA6 + 30% GF
Tensile strengthMPa70147129
Elongation at break%451013
Flexural strengthMPa78218167
Flexural modulusMPa234585406210
Notched impact strengthkJ/m²5.51413
Unnotched impact strengthkJ/m²1305557

Swipe to compare all columns ↔

PA6: 20% glass fibre + 20% mineral filler
PropertyStandard / conditionUnitWhiskerWollastonite
Tensile strengthASTM D638-2010MPa95.977.0
Flexural strengthASTM D790-2010MPa216178
Flexural modulusASTM D790-2010MPa1352813862
Notched impact strengthASTM D256-2010J/m10286

Trade-offs remain: 30% whisker reduces notched impact from 4.72 to 3.4; the hybrid lowers elongation from 13% to 10% and unnotched impact from 57 to 55 kJ/m² versus 30% glass fibre; whiskers give a lower flexural modulus than wollastonite, 13528 versus 13862 MPa. Verify stiffness, toughness and processing together. The first table retains the source units without conversion; the second supplies no standards.

02Source and conditions

Source: 超细纤维添加各个行业的测试数据.pdf, PDF pp. 3. Test date not supplied. No named testing organisation or report number is given.

These records compare the listed formulations and are not guaranteed values for every grade. Full raw-material grades, batches, specimen counts and repeatability are not supplied. Repeat the trials with the intended materials and process.

Full test report ↗
1 data tablesPBAT film: 30% and 45% filler and masterbatch comparison

Four film groups retain thickness, directional tensile, elongation, tear and puncture data. Higher filler loading does not improve every mechanical property.

Process
masterbatch / direct film blowing

PBAT-1: 30% filler; PBAT-2 and PBAT-3: 45%; PBAT-4: 30%, using a 75%-filled masterbatch mixed at 1:1.5 before film blowing. The filler is a whisker/calcium-carbonate system with an unspecified internal ratio. Other differences between PBAT-2 and PBAT-3 are not explained.

Swipe to compare all columns ↔

Full data for four PBAT film groups
PropertyUnitPBAT-1PBAT-2PBAT-3PBAT-4Standard / condition
Thicknessmm0.040.040.050.05—
Transverse tensile strengthMPa16.218.9110.7915.09GB/T 1040.3; 23°C; 200 mm/min
Transverse strain at break%608452520731GB/T 1040.3; 23°C; 200 mm/min
Longitudinal tensile strengthMPa18.0112.6913.0019.38GB/T 1040.3; 23°C; 200 mm/min
Longitudinal strain at break%218163205380GB/T 1040.3; 23°C; 200 mm/min
Transverse tear strengthkN/m83.5059.0563.8484.84QB/T 1130; 23°C; 200 mm/min
Longitudinal tear strengthkN/m86.3569.3072.3273.20QB/T 1130; 23°C; 200 mm/min
Puncture forceN1.080.770.971.09GB/T 37841; 23°C; 50 mm/min

Versus PBAT-1, PBAT-2 drops from 16.21 to 8.91 MPa in transverse strength and from 1.08 to 0.77 N in puncture force. PBAT-4 has higher longitudinal strength but lower longitudinal tear strength, 86.35→73.20 kN/m, with thickness increasing from 0.04 to 0.05 mm. Do not select a formulation by a single maximum. The source prose and tabulated film thickness differ in magnitude; only the specimen-table thicknesses are used here.

This is a mechanical and processing reference. No degradation rate, composting conditions or related certification is supplied; it does not establish certified biodegradability of the finished product.

02Source and conditions

Source: 超细纤维添加各个行业的测试数据.pdf, PDF pp. 8. Test date not supplied. No named testing organisation or report number is given.

These records compare the listed formulations and are not guaranteed values for every grade. Full raw-material grades, batches, specimen counts and repeatability are not supplied. Repeat the trials with the intended materials and process.

Full test report ↗