Selection parameters
- Validation
- matrix/process dependent
01Validation route
Confirm the matrix, target properties and process window, then select surface treatment, run a dosage gradient and retest performance. Published data does not replace customer-specific validation.
APPLICATION EVIDENCE
Application test data
These records relate to this application. Formulations, loadings and conditions differ; review the complete comparisons.
1 data tablesFlame-retardant nylon: 5%, 10% and 15% whisker comparison
The 10% formulation has the highest tensile, flexural and notched-impact values in this set; 15% gives no further gain. The source combines PA6/PA66 and describes replacement of halogenated flame retardant.
- Filler loading
- 5 / 10 / 15 %
Trial objective: replace part of a halogenated flame retardant with whiskers, comparing baseline, 5%, 10% and 15% formulations. PA6 and PA66 are not reported separately. The percentage basis and flame-retardant grade are unspecified.
Swipe to compare all columns ↔
| Property | Standard / condition | Unit | Baseline | 5% | 10% | 15% |
|---|---|---|---|---|---|---|
| Density | ISO 1183 | g/cm³ | 1.58 | 1.50 | 1.53 | 1.55 |
| Tensile strength | ISO 527 | MPa | 104 | 117 | 125 | 124 |
| Elongation at break | ISO 527 | % | 5.0 | 5.2 | 6.5 | 6.2 |
| Flexural strength | ISO 178 | MPa | 139 | 157 | 173 | 167 |
| Flexural modulus | ISO 178 | MPa | 5800 | 6450 | 6700 | 6600 |
| Notched impact strength | ISO 180 | kJ/m² | 8.1 | 10.2 | 11.3 | 10.6 |
| Glow-wire recorded time | IEC 60695 | s | 6 | 5 | 3 | 5 |
| Glow-wire ignition observation | IEC 60695 | — | No ignition reported | No ignition reported | No ignition reported | No ignition reported |
| Vertical burning rating | UL 94 | — | V0 | V0 | V0 | V0 |
| Heat deflection temperature | ISO 75 | °C | 202 | 202 | 203 | 203 |
At 10%, tensile strength rises from 104 to 125 MPa, flexural strength from 139 to 173 MPa, and notched impact from 8.1 to 11.3 kJ/m². At 15%, they fall back to 124, 167 and 10.6. Verify cost and performance in the customer formulation; 10% is not a universal optimum.
Standard editions, glow-wire temperature, UL 94 specimen thickness and HDT load are not supplied. V0 is the recorded rating, not a product certification. The source unit “Glass” for vertical burning is presented here as a rating.
02Source and conditions
Source: 超细纤维添加各个行业的测试数据.pdf, PDF pp. 2. Test date: 2025-07-16. No named testing organisation or report number is given.
These records compare the listed formulations and are not guaranteed values for every grade. Full raw-material grades, batches, specimen counts and repeatability are not supplied. Repeat the trials with the intended materials and process.
1 data tablesPA6/PA66 nylon: 8% whisker replacement of halogen-free flame retardant
The 8% formulation records tensile strength of 100→103 MPa, flexural strength of 115→125 MPa and notched impact of 9.5→10.2 kJ/m²; density rises from 1.40 to 1.41 g/mL.
- Filler loading
- 8 %
This record has a different flame-retardant system, baseline, date and standards from the 5%/10%/15% trial. Read it separately. The title names both PA6 and PA66 without separate results.
Swipe to compare all columns ↔
| Property | Standard / condition | Unit | Baseline | 8% |
|---|---|---|---|---|
| Density | GB/T 1033 | g/mL | 1.40 | 1.41 |
| Tensile strength | GB/T 1040 | MPa | 100 | 103 |
| Elongation at break | GB/T 1040 | % | 7 | 7.5 |
| Flexural strength | GB/T 9341 | MPa | 115 | 125 |
| Flexural modulus | GB/T 9341 | MPa | 5600 | 5800 |
| Notched impact strength | GB/T 1843 | kJ/m² | 9.5 | 10.2 |
| Ash / glass-fibre content (source label) | GB/1635 | % | 33.5 | 33 |
| Glow-wire time at 880°C | GB/T 5169 | s | 10 | 10 |
| Glow-wire observation at 760°C | GB/T 5169 | — | No burning reported | No burning reported |
| Vertical burning rating | UL 94 | T1 / T2 | V0 | V0 |
The ash / glass-fibre standard is printed “GB/1635” and is retained without substituting another standard. UL 94 specimen thickness, full glow-wire criteria, standard editions and dosage basis are not provided. V0 is not an independent certification claim.
02Source and conditions
Source: 超细纤维添加各个行业的测试数据.pdf, PDF pp. 1. Test date: 2025-08-25. No named testing organisation or report number is given.
These records compare the listed formulations and are not guaranteed values for every grade. Full raw-material grades, batches, specimen counts and repeatability are not supplied. Repeat the trials with the intended materials and process.
3 data tablesPA6: whisker, glass-fibre and wollastonite comparisons
The 15% glass-fibre + 15% whisker group has higher strength but lower elongation and unnotched impact than the 30% glass-fibre group. Three source tables are kept separate.
These three comparisons use different formulations and units and must not be ranked across tables. The first says nylon without a PA grade; the second specifies unactivated whiskers; the third compares equal loadings of whiskers and wollastonite.
Swipe to compare all columns ↔
| Property | Standard / condition | Unit | Blank | 30% |
|---|---|---|---|---|
| Tensile strength | D638 | kg/cm² | 635 | 835 |
| Tensile modulus | D638 | kg/cm² | 2.33×10⁴ | 4.53×10⁴ |
| Flexural strength | D790 | kg/cm² | 879 | 1208 |
| Flexural modulus | D790 | kg/cm² | 2.13×10⁴ | 4.03×10⁴ |
| Notched impact strength | D256 | kgf·cm/cm | 4.72 | 3.4 |
| Heat deflection temperature | D648 | °C | 65 | 90.5 |
Swipe to compare all columns ↔
| Property | Unit | 100% PA6 | PA6 + 15% GF + 15% CSW | PA6 + 30% GF |
|---|---|---|---|---|
| Tensile strength | MPa | 70 | 147 | 129 |
| Elongation at break | % | 45 | 10 | 13 |
| Flexural strength | MPa | 78 | 218 | 167 |
| Flexural modulus | MPa | 2345 | 8540 | 6210 |
| Notched impact strength | kJ/m² | 5.5 | 14 | 13 |
| Unnotched impact strength | kJ/m² | 130 | 55 | 57 |
Swipe to compare all columns ↔
| Property | Standard / condition | Unit | Whisker | Wollastonite |
|---|---|---|---|---|
| Tensile strength | ASTM D638-2010 | MPa | 95.9 | 77.0 |
| Flexural strength | ASTM D790-2010 | MPa | 216 | 178 |
| Flexural modulus | ASTM D790-2010 | MPa | 13528 | 13862 |
| Notched impact strength | ASTM D256-2010 | J/m | 102 | 86 |
Trade-offs remain: 30% whisker reduces notched impact from 4.72 to 3.4; the hybrid lowers elongation from 13% to 10% and unnotched impact from 57 to 55 kJ/m² versus 30% glass fibre; whiskers give a lower flexural modulus than wollastonite, 13528 versus 13862 MPa. Verify stiffness, toughness and processing together. The first table retains the source units without conversion; the second supplies no standards.
02Source and conditions
Source: 超细纤维添加各个行业的测试数据.pdf, PDF pp. 3. Test date not supplied. No named testing organisation or report number is given.
These records compare the listed formulations and are not guaranteed values for every grade. Full raw-material grades, batches, specimen counts and repeatability are not supplied. Repeat the trials with the intended materials and process.
3 data tablesPP and HDPE: drawing, automotive and injection-moulding comparisons
Three separate datasets cover PP drawing, PP automotive parts and HDPE, retaining toughness and flow changes alongside stiffness gains for realistic substitution decisions.
- Material systems
- PP / HDPE
- Evaluation focus
- modulus, impact, thickness, cost
01PP drawing and weaving
Loading and filament thickness both vary in this table. Strength changes cannot be attributed to whiskers alone, nor converted into a universal cost-saving percentage.
Swipe to compare all columns ↔
| Property | Unit | CaCO₃-filled PP | Whisker PP: 25% | Whisker PP: 40% |
|---|---|---|---|---|
| Filler loading | % | 18 | 25 | 40 |
| Monofilament strength | MPa | 270–310 | 340 | 290 |
| Monofilament maximum force | N | 30–35 | 35 | 24 |
| Thickness | mm | 0.045 | 0.040 | 0.036 |
02PP automotive formulations
PP-1: 20% talc; PP-2: 10% whisker + 10% calcium carbonate; PP-3: 20% whisker.
Swipe to compare all columns ↔
| Property | Unit | PP-1 | PP-2 | PP-3 | Standard / condition |
|---|---|---|---|---|---|
| Tensile strength | MPa | 21.4 | 20.5 | 22.2 | GB/T 1040.2; 23°C; 50 mm/min |
| Elongation at break | % | 67 | 62 | 27 | GB/T 1040.2; 23°C; 50 mm/min |
| Flexural strength | MPa | 28.3 | 27.6 | 29.7 | GB/T 9341; 23°C; 2 mm/min |
| Flexural modulus | MPa | 1637 | 1691 | 2053 | GB/T 9341; 23°C; 2 mm/min |
| Notched impact strength | kJ/m² | 7.5 | 7.4 | 6.5 | GB/T 1843; 23°C; A |
| Melt mass-flow rate (MFR) | g/10 min | 15.361 | 14.655 | 16.64 | GB/T 3682.1; 230°C; 2.16 kg |
Versus PP-1, PP-3 raises flexural modulus from 1637 to 2053 MPa but reduces elongation from 67% to 27% and notched impact from 7.5 to 6.5 kJ/m². Substitution depends on part impact requirements and surface quality.
03HDPE injection and product validation
PE-1: 20% talc + 20% calcium carbonate; PE-2: 20% whisker + 20% calcium carbonate; PE-3: 20% whisker + 20% talc.
Swipe to compare all columns ↔
| Property | Unit | PE-1 | PE-2 | PE-3 | Standard / condition |
|---|---|---|---|---|---|
| Flexural strength | MPa | 20.9 | 22 | 24.9 | GB/T 9341; 23°C; 2 mm/min |
| Flexural modulus | MPa | 1396 | 1822 | 1877 | GB/T 9341; 23°C; 2 mm/min |
| Notched impact strength | kJ/m² | 44.7 | 48.2 | 11.7 | GB/T 1843; 23°C; A |
| Melt mass-flow rate (MFR) | g/10 min | 0.3089 | 0.3150 | 0.1161 | GB/T 3682.1; 190°C; 5 kg |
PE-2 improves both flexural modulus and notched impact versus PE-1. PE-3 has a higher modulus but notched impact falls to 11.7 kJ/m² and MFR to 0.1161 g/10 min. Its 1877 MPa modulus alone is insufficient for a recommendation.
Page 7 describes blow-moulded pallets and corrugated-pipe trials without full product reports, standard identifiers or cost breakdowns. Its compliance and cost statements are not universal product promises. Verify loading, drop resistance, ring stiffness and cost per acceptable part before thinning or substitution.
04Source and conditions
Source: 超细纤维添加各个行业的测试数据.pdf, PDF pp. 4, 5, 6, 7. Test date not supplied. No named testing organisation or report number is given.
These records compare the listed formulations and are not guaranteed values for every grade. Full raw-material grades, batches, specimen counts and repeatability are not supplied. Repeat the trials with the intended materials and process.
1 data tablesPBAT film: 30% and 45% filler and masterbatch comparison
Four film groups retain thickness, directional tensile, elongation, tear and puncture data. Higher filler loading does not improve every mechanical property.
- Process
- masterbatch / direct film blowing
PBAT-1: 30% filler; PBAT-2 and PBAT-3: 45%; PBAT-4: 30%, using a 75%-filled masterbatch mixed at 1:1.5 before film blowing. The filler is a whisker/calcium-carbonate system with an unspecified internal ratio. Other differences between PBAT-2 and PBAT-3 are not explained.
Swipe to compare all columns ↔
| Property | Unit | PBAT-1 | PBAT-2 | PBAT-3 | PBAT-4 | Standard / condition |
|---|---|---|---|---|---|---|
| Thickness | mm | 0.04 | 0.04 | 0.05 | 0.05 | — |
| Transverse tensile strength | MPa | 16.21 | 8.91 | 10.79 | 15.09 | GB/T 1040.3; 23°C; 200 mm/min |
| Transverse strain at break | % | 608 | 452 | 520 | 731 | GB/T 1040.3; 23°C; 200 mm/min |
| Longitudinal tensile strength | MPa | 18.01 | 12.69 | 13.00 | 19.38 | GB/T 1040.3; 23°C; 200 mm/min |
| Longitudinal strain at break | % | 218 | 163 | 205 | 380 | GB/T 1040.3; 23°C; 200 mm/min |
| Transverse tear strength | kN/m | 83.50 | 59.05 | 63.84 | 84.84 | QB/T 1130; 23°C; 200 mm/min |
| Longitudinal tear strength | kN/m | 86.35 | 69.30 | 72.32 | 73.20 | QB/T 1130; 23°C; 200 mm/min |
| Puncture force | N | 1.08 | 0.77 | 0.97 | 1.09 | GB/T 37841; 23°C; 50 mm/min |
Versus PBAT-1, PBAT-2 drops from 16.21 to 8.91 MPa in transverse strength and from 1.08 to 0.77 N in puncture force. PBAT-4 has higher longitudinal strength but lower longitudinal tear strength, 86.35→73.20 kN/m, with thickness increasing from 0.04 to 0.05 mm. Do not select a formulation by a single maximum. The source prose and tabulated film thickness differ in magnitude; only the specimen-table thicknesses are used here.
This is a mechanical and processing reference. No degradation rate, composting conditions or related certification is supplied; it does not establish certified biodegradability of the finished product.
02Source and conditions
Source: 超细纤维添加各个行业的测试数据.pdf, PDF pp. 8. Test date not supplied. No named testing organisation or report number is given.
These records compare the listed formulations and are not guaranteed values for every grade. Full raw-material grades, batches, specimen counts and repeatability are not supplied. Repeat the trials with the intended materials and process.