Test conditions
- Surface treatment
- KH-550 where stated
- Material systems
- epoxy / SBS / PU / tile adhesive
Seven examples cover epoxy, structural adhesives, SBS, polyurethane-modified epoxy, tile adhesive and polyurethane. Matrices, dosage bases and test conditions differ, so absolute strengths must not be compared across examples. CSW means calcium sulphate whisker; KCSW is KH-550-treated whisker.
021. Epoxy filler record: units need verification
Page 17 lists 100 g E-44 epoxy, 20 g per filler and KH-550 as 20 g × 1%. It does not clearly distinguish separate filler formulations from simultaneous addition, and labels strengths in GPa. These are raw records pending clarification, not performance claims; the units have not been silently changed to MPa.
Swipe to compare all columns ↔
| Filler | Tensile strength | Shear strength | Unit |
|---|---|---|---|
| Calcium sulphate whisker | 26.4 | 22.8 | Source says GPa; unit unverified |
| Quartz powder | 11.9 | 9.2 | Source says GPa; unit unverified |
| Alumina powder | 16.9 | 11.1 | Source says GPa; unit unverified |
| Silica | 17.0 | 16.1 | Source says GPa; unit unverified |
| Ultrafine aluminium silicate | 17.2 | 16.2 | Source says GPa; unit unverified |
032. Structural adhesive comparison
On page 18, the improved group adds KH-550-treated whiskers to a silica-powder filler. Component weights are absent. The source writes “mPa”; that notation is retained pending confirmation and is not suitable for engineering selection.
Swipe to compare all columns ↔
| Adhesive / group | Shear strength | Tensile strength | Compressive strength |
|---|---|---|---|
| Steel-bonding / control | 20.88 | 35.48 | 71.84 |
| Steel-bonding / improved | 24.90 | 38.90 | 77.88 |
| Rebar anchoring / control | 19.68 | 35.55 | 73.76 |
| Rebar anchoring / improved | 21.46 | 35.58 | 78.60 |
043. Epoxy surface treatment and quartz blend
Swipe to compare all columns ↔
| Formulation | Epoxy resin | CSW | KCSW | Quartz powder |
|---|---|---|---|---|
| 1 | 100 | 10 | 0 | 0 |
| 2 | 100 | 10 | 0 | 20 |
| 3 | 100 | 0 | 10 | 20 |
Swipe to compare all columns ↔
| Formulation | Tensile strength | Shear strength |
|---|---|---|
| 1 | 17.8 | 16.9 |
| 2 | 25.0 | 20.0 |
| 3 | 31.0 | 24.4 |
054. SBS adhesive
Swipe to compare all columns ↔
| Formulation | SBS | Tackifying resin | Rosin resin | CSW | KCSW | Solvent |
|---|---|---|---|---|---|---|
| 1 | 10 | 6 | 7 | 0 | 0 | 20–40 |
| 2 | 10 | 6 | 7 | 6 | 0 | 20–40 |
| 3 | 10 | 6 | 7 | 0 | 6 | 20–40 |
Swipe to compare all columns ↔
| Formulation | T-peel strength (N/m) | Source-reported increase |
|---|---|---|
| 1 | 589.5 | 0 |
| 2 | 694.8 | 17.86% |
| 3 | 723.7 | 22.77% |
The page-19 SBS entries do not form a complete 100% formulation, and solvent is only given as a 20–40% range. They indicate a comparison direction, not a production-ready recipe.
065. Polyurethane-modified epoxy
The recipe gives 100 parts polyurethane-modified epoxy plus 10–15 parts modified whisker, while the results label 10% and 15%. Their relationship is not explained, so both source notations are retained.
Swipe to compare all columns ↔
| Source dosage | Room-temperature shear | Shear at −70°C | Shear at 100°C | Peel |
|---|---|---|---|---|
| 10% | 5% | 10% | — | 27% |
| 15% | 15% | — | 39% | — |
076. Tile adhesive reference
Page 20 gives ranges: white cement 35–60%, quartz sand 20–30%, ground calcium carbonate 18–35%, HPMC 0.1–0.4%, whisker 0.4–0.5%, water reducer 0.2–1.0%, latex powder 2–3%, lignocellulose 0.5–1.0%, high-alumina cement 0.5–0.8%; colourant amount is absent. Do not combine every upper limit into a recipe.
Swipe to compare all columns ↔
| Property | Unit | Recorded result |
|---|---|---|
| Appearance | — | Homogeneous dry powder, no lumps |
| Compressive strength, 3 d | mPa* | 10.0 |
| Water impermeability, 7 d, 3 mm coating | mPa* | 0.8 |
| Initial setting time | min | 353 |
| Final setting time | min | 605 |
| Bond strength, 7 d: value unverified | mPa* | 114 |
| Flexural strength, 7 d | mPa* | 4.2 |
| Water resistance (criterion absent) | % | 80 |
| Alkali resistance: 10% NaOH, 48 h immersion | — | No cracking, shelling or peeling reported |
* The source unit mPa and the 7-day bond value “114” require confirmation. Neither has been silently changed to MPa or 1.14; they are not marketing or engineering commitments.
087. Polyurethane adhesive
The recipe lists 97% polyurethane and 3% KH-550-modified whisker. Source units are mPa for tensile strength, mPa·s for viscosity and KN/m for peel. They are retained below pending confirmation.
Swipe to compare all columns ↔
| Property | Unit | 0% | 3% |
|---|---|---|---|
| Tensile strength | mPa* | 40 | 56 |
| Initial adhesion strength | KN/m* | 2.6 | 3.8 |
| Peel strength | KN/m* | 5.6 | 8.5 |
| Viscosity | mPa·s | 1500 | 1650 |
| Solids content | % | 20 | 21.6 |
Viscosity increases at 3%, so application behaviour must also be assessed. Comparing only 0% and 3% does not establish a universal optimum. Full standards, cure conditions and specimen counts are absent for these examples; establish them before customer replication.
09Source and conditions
Source: 超细纤维添加各个行业的测试数据.pdf, PDF pp. 17, 18, 19, 20. Test date not supplied. No named testing organisation or report number is given.
These records compare the listed formulations and are not guaranteed values for every grade. Full raw-material grades, batches, specimen counts and repeatability are not supplied. Repeat the trials with the intended materials and process.