Test conditions
- Filler loading
- 5 / 10 / 15 %
Trial objective: replace part of a halogenated flame retardant with whiskers, comparing baseline, 5%, 10% and 15% formulations. PA6 and PA66 are not reported separately. The percentage basis and flame-retardant grade are unspecified.
Swipe to compare all columns ↔
| Property | Standard / condition | Unit | Baseline | 5% | 10% | 15% |
|---|---|---|---|---|---|---|
| Density | ISO 1183 | g/cm³ | 1.58 | 1.50 | 1.53 | 1.55 |
| Tensile strength | ISO 527 | MPa | 104 | 117 | 125 | 124 |
| Elongation at break | ISO 527 | % | 5.0 | 5.2 | 6.5 | 6.2 |
| Flexural strength | ISO 178 | MPa | 139 | 157 | 173 | 167 |
| Flexural modulus | ISO 178 | MPa | 5800 | 6450 | 6700 | 6600 |
| Notched impact strength | ISO 180 | kJ/m² | 8.1 | 10.2 | 11.3 | 10.6 |
| Glow-wire recorded time | IEC 60695 | s | 6 | 5 | 3 | 5 |
| Glow-wire ignition observation | IEC 60695 | — | No ignition reported | No ignition reported | No ignition reported | No ignition reported |
| Vertical burning rating | UL 94 | — | V0 | V0 | V0 | V0 |
| Heat deflection temperature | ISO 75 | °C | 202 | 202 | 203 | 203 |
At 10%, tensile strength rises from 104 to 125 MPa, flexural strength from 139 to 173 MPa, and notched impact from 8.1 to 11.3 kJ/m². At 15%, they fall back to 124, 167 and 10.6. Verify cost and performance in the customer formulation; 10% is not a universal optimum.
Standard editions, glow-wire temperature, UL 94 specimen thickness and HDT load are not supplied. V0 is the recorded rating, not a product certification. The source unit “Glass” for vertical burning is presented here as a rating.
02Source and conditions
Source: 超细纤维添加各个行业的测试数据.pdf, PDF pp. 2. Test date: 2025-07-16. No named testing organisation or report number is given.
These records compare the listed formulations and are not guaranteed values for every grade. Full raw-material grades, batches, specimen counts and repeatability are not supplied. Repeat the trials with the intended materials and process.