These three comparisons use different formulations and units and must not be ranked across tables. The first says nylon without a PA grade; the second specifies unactivated whiskers; the third compares equal loadings of whiskers and wollastonite.

Swipe to compare all columns ↔

Nylon: unfilled versus 30% whisker
PropertyStandard / conditionUnitBlank30%
Tensile strengthD638kg/cm²635835
Tensile modulusD638kg/cm²2.33×10⁴4.53×10⁴
Flexural strengthD790kg/cm²8791208
Flexural modulusD790kg/cm²2.13×10⁴4.03×10⁴
Notched impact strengthD256kgf·cm/cm4.723.4
Heat deflection temperatureD648°C6590.5

Swipe to compare all columns ↔

PA6: 15% glass fibre + 15% unactivated whisker versus 30% glass fibre
PropertyUnit100% PA6PA6 + 15% GF + 15% CSWPA6 + 30% GF
Tensile strengthMPa70147129
Elongation at break%451013
Flexural strengthMPa78218167
Flexural modulusMPa234585406210
Notched impact strengthkJ/m²5.51413
Unnotched impact strengthkJ/m²1305557

Swipe to compare all columns ↔

PA6: 20% glass fibre + 20% mineral filler
PropertyStandard / conditionUnitWhiskerWollastonite
Tensile strengthASTM D638-2010MPa95.977.0
Flexural strengthASTM D790-2010MPa216178
Flexural modulusASTM D790-2010MPa1352813862
Notched impact strengthASTM D256-2010J/m10286

Trade-offs remain: 30% whisker reduces notched impact from 4.72 to 3.4; the hybrid lowers elongation from 13% to 10% and unnotched impact from 57 to 55 kJ/m² versus 30% glass fibre; whiskers give a lower flexural modulus than wollastonite, 13528 versus 13862 MPa. Verify stiffness, toughness and processing together. The first table retains the source units without conversion; the second supplies no standards.

02Source and conditions

Source: 超细纤维添加各个行业的测试数据.pdf, PDF pp. 3. Test date not supplied. No named testing organisation or report number is given.

These records compare the listed formulations and are not guaranteed values for every grade. Full raw-material grades, batches, specimen counts and repeatability are not supplied. Repeat the trials with the intended materials and process.