Test conditions
- Material systems
- PP / HDPE
- Evaluation focus
- modulus, impact, thickness, cost
01PP drawing and weaving
Loading and filament thickness both vary in this table. Strength changes cannot be attributed to whiskers alone, nor converted into a universal cost-saving percentage.
Swipe to compare all columns ↔
| Property | Unit | CaCO₃-filled PP | Whisker PP: 25% | Whisker PP: 40% |
|---|---|---|---|---|
| Filler loading | % | 18 | 25 | 40 |
| Monofilament strength | MPa | 270–310 | 340 | 290 |
| Monofilament maximum force | N | 30–35 | 35 | 24 |
| Thickness | mm | 0.045 | 0.040 | 0.036 |
02PP automotive formulations
PP-1: 20% talc; PP-2: 10% whisker + 10% calcium carbonate; PP-3: 20% whisker.
Swipe to compare all columns ↔
| Property | Unit | PP-1 | PP-2 | PP-3 | Standard / condition |
|---|---|---|---|---|---|
| Tensile strength | MPa | 21.4 | 20.5 | 22.2 | GB/T 1040.2; 23°C; 50 mm/min |
| Elongation at break | % | 67 | 62 | 27 | GB/T 1040.2; 23°C; 50 mm/min |
| Flexural strength | MPa | 28.3 | 27.6 | 29.7 | GB/T 9341; 23°C; 2 mm/min |
| Flexural modulus | MPa | 1637 | 1691 | 2053 | GB/T 9341; 23°C; 2 mm/min |
| Notched impact strength | kJ/m² | 7.5 | 7.4 | 6.5 | GB/T 1843; 23°C; A |
| Melt mass-flow rate (MFR) | g/10 min | 15.361 | 14.655 | 16.64 | GB/T 3682.1; 230°C; 2.16 kg |
Versus PP-1, PP-3 raises flexural modulus from 1637 to 2053 MPa but reduces elongation from 67% to 27% and notched impact from 7.5 to 6.5 kJ/m². Substitution depends on part impact requirements and surface quality.
03HDPE injection and product validation
PE-1: 20% talc + 20% calcium carbonate; PE-2: 20% whisker + 20% calcium carbonate; PE-3: 20% whisker + 20% talc.
Swipe to compare all columns ↔
| Property | Unit | PE-1 | PE-2 | PE-3 | Standard / condition |
|---|---|---|---|---|---|
| Flexural strength | MPa | 20.9 | 22 | 24.9 | GB/T 9341; 23°C; 2 mm/min |
| Flexural modulus | MPa | 1396 | 1822 | 1877 | GB/T 9341; 23°C; 2 mm/min |
| Notched impact strength | kJ/m² | 44.7 | 48.2 | 11.7 | GB/T 1843; 23°C; A |
| Melt mass-flow rate (MFR) | g/10 min | 0.3089 | 0.3150 | 0.1161 | GB/T 3682.1; 190°C; 5 kg |
PE-2 improves both flexural modulus and notched impact versus PE-1. PE-3 has a higher modulus but notched impact falls to 11.7 kJ/m² and MFR to 0.1161 g/10 min. Its 1877 MPa modulus alone is insufficient for a recommendation.
Page 7 describes blow-moulded pallets and corrugated-pipe trials without full product reports, standard identifiers or cost breakdowns. Its compliance and cost statements are not universal product promises. Verify loading, drop resistance, ring stiffness and cost per acceptable part before thinning or substitution.
04Source and conditions
Source: 超细纤维添加各个行业的测试数据.pdf, PDF pp. 4, 5, 6, 7. Test date not supplied. No named testing organisation or report number is given.
These records compare the listed formulations and are not guaranteed values for every grade. Full raw-material grades, batches, specimen counts and repeatability are not supplied. Repeat the trials with the intended materials and process.